Defects and preventive measures of stamping and stretching parts
Time : 2023-08-30 Click count : 2648

1. Reasons for waste generation:

A. Poor quality of raw materials;

B. Improper installation, adjustment, and use of molds;

C. The worker did not feed the strip correctly along the positioning or did not ensure that the strip was fed with a certain gap;

D. Due to long-term use of the mold, there may be changes in gaps or wear on the working and guiding components of the mold;

E. Due to prolonged impact and vibration, the fastening parts of the mold become loose, causing a relative change in the installation position of the mold;

F. The operator's negligence did not follow the operating procedures.


2. The main measures to prevent waste are:

A. Raw materials must meet the specified technical conditions (strictly inspect the specifications and brands of raw materials, and conduct laboratory tests on workpieces with high requirements for dimensional accuracy and surface quality when conditions permit)

B. All aspects specified in the process specifications should be strictly followed comprehensively;

C. The tools and equipment used, such as presses and molds, should ensure that they work under normal working conditions;

D. Establish a strict inspection system during the production process, which requires a thorough inspection of the first stamped part. Only after passing the inspection can they be put into production. At the same time, inspection should be strengthened, and accidents should be dealt with in a timely manner;

E. Adhere to the civilized production system, for example, workpieces and blanks must be transported using appropriate workstation equipment, otherwise the surface of the workpiece will be crushed and scratched, affecting the surface quality of the workpiece;

F. During the stamping process, the cleanliness of the mold cavity should be ensured, and the orderly arrangement of workpieces after processing in the workplace should be neat.


3. Causes of burrs on punched parts

A. The punching gap is too large, too small, or uneven;

B. The cutting edge of the working part of the mold becomes dull;

C. Due to long-term vibration impact, the centerlines of the convex and concave molds change, and the axes do not coincide, resulting in one-sided burrs.

measures:

1) Ensure the machining accuracy and assembly quality of convex and concave molds, ensure the verticality of convex molds, withstand lateral pressure, and ensure the rigidity of the entire mold;

2) When installing the convex mold, ensure that the gap between the convex mold and the concave mold is correct, and firmly install the convex mold and the concave mold on the mold fixing plate. The end faces of the upper and lower molds should be parallel to the worktable of the press.

3) The requirements for the press include good rigidity, minimal elastic deformation, high track accuracy, and high parallelism between the pad and slider;

4) Require the pressure machine to have sufficient punching force.

The allowable height of burrs on the cut surface of punched parts

Punched sheet thickness>0.3>0.3-0.5>0.5-1.0>1.0-1.5>1.5-2.0

New trial mold burr height ≤ 0.015 ≤ 0.02 ≤ 0.03 ≤ 0.04 ≤ 0.05

The allowable burr height in production is ≤ 0.05 ≤ 0.08 ≤ 0.10 ≤ 0.13 ≤ 0.15


4. Reasons for warping and deformation of punched parts:

There are clearance forces and reaction forces on a straight line that do not generate torque. When the gap between the punch and the die is too large, the edge of the die has a conical shape, or when the contact area between the ejector and the workpiece is too small, warping deformation will occur

measures:

A. Reasonably choose the punching gap;

B. In the mold structure, a certain amount of pressure is required to increase the plane contact between the pressing plate (or support plate) and the pressing plate;

C. Check the concave die blade. If a reverse taper is found, the cutting edge of the die must be trimmed correctly.

D. When the shape of the punched part is complex and there are many inner holes, if the cutting force is uneven, the pressing force will increase. Before punching, press the strip tightly or use a high-precision press to punch it.

E. Before punching the sheet metal, it should be leveled. If the warping cannot be removed, the punched workpiece can be re leveled using a leveling mold.

F. Regularly clean the dirt inside the mold cavity, lubricate the surface of the thin sheet material, and install oil vent holes on the mold structure.


5. During punching, the accuracy of the outer edge and inner hole of the punched part decreases, and the size changes.

reason:

The position of positioning pins, blocking pins, etc. has changed or worn out excessively;

The operator's carelessness caused the material to move back and forth during feeding;

The dimensional accuracy of the strip material is low, too narrow and too wide, making it difficult to deliver to the designated location. If the strip material moves back and forth in the guide plate, the punching hole of the workpiece will have a significant deviation from the front and rear positions of the outer shape.


6. Reasons for non-conforming bending dimensions and shapes of parts

A. The rebound of the material causes the product to be unqualified

Measures to reduce rebound:

Choose stamping materials with stable mechanical properties, high elastic modulus, and low yield point;

Add calibration program and use calibration bending instead of free bending;

Before bending, the material should be annealed to soften the cold work hardened material before bending into shape;

If there is shape deformation during stamping, it is difficult to remove; Then change or adjust the slope of the convex and concave molds, and the gap between the convex and concave molds should be equal to the minimum material thickness.

Increase the contact area between the concave mold and the workpiece, and reduce the contact area between the convex mold and the workpiece.

Reduce the impact of rebound by overcorrecting.

B. If the locator is worn and deformed, causing inaccurate positioning of the strip, a new locator must be replaced.

C. In non guided bending molds, improper adjustment of the bottom dead center position of the press slide during adjustment on the press can also result in the shape and size of the bent part being non-conforming.

D. If the pressing device of the mold malfunctions or does not work at all, it is necessary to readjust the pressing force or replace the pressure spring to make it work normally.


7. Cracks appear at the bending part of the bent part (the internal stress in the bending deformation zone exceeds the material strength limit)

A. Removing burrs outside the curved area can lead to stress concentration in that area,

1) Reduce bending deformation

2) Remove burrs from the area

3) Place the side with burrs inside the curved area

B. When bending workpieces, it is best to make the bending direction perpendicular to the fiber direction (rolling direction) of the material.

C. The bending radius should not be too small, and if the quality allows, the fillet radius should be increased as much as possible.

D. The surface of the bent blank should be smooth, without obvious protrusions or scars.

E. Intermediate annealing process is used to remove internal stress during bending, and softening bending rarely produces cracks.

F. When bending, larger bending parts must be coated with lubricant to reduce friction during bending.


8. Deviation of bent parts during bending process

During the bending process, when the blank slides along the surface of the concave mold, it will experience frictional resistance. If the frictional resistance on both sides of the blank is significantly different, the blank will move towards the side with greater frictional resistance.

measures:

1) Asymmetric bending parts are formed by symmetrical bending (single-sided bending parts are cut after two symmetrical bends)

2) Add an elastic compression device on the bending mold to compress the billet and prevent it from moving during bending.

3) Utilize internal holes and external positioning forms to ensure accurate positioning.


9. Reasons and solutions for surface scratches on curved parts.

A. When continuously bending soft materials such as copper and aluminum alloys, metal particles or slag are prone to adhere to the surface of the working area, causing significant scratches on the parts. At this time, it is necessary to carefully analyze and study the shape and lubricating oil of the working parts, and it is best to avoid particles and slag on the blank, which can cause scratches.

B. When the bending direction is parallel to the rolling direction of the material, cracks will appear on the surface of the workpiece, reducing the surface quality of the workpiece. When two or more parts are bent, ensure that the bending direction is as close as possible to the rolling direction.

C. When the burr surface is bent as the outer surface, the parts are prone to cracking and scratching; Therefore, the burr surface should be considered as a curved inner surface.

D. The fillet radius of the concave mold is too small, and there are impact marks on the curved part. Polishing the concave mold and increasing the fillet radius of the concave mold can avoid wear on bent parts.

E. The gap between the convex and concave molds should not be too small, otherwise it will cause thinning and wear. Regularly check the changes in mold clearance during stamping.

F. If the depth of the convex mold entering the concave mold is too large, there may be scratches on the surface of the part. Therefore, while ensuring that it is not affected by rebound, the depth of the convex mold entering the concave mold should be appropriately reduced.

G. In order to meet the precision requirements of the parts, bottom pressing bending molds are often used. When bending, the springs, locating pin holes, support plates, and return holes on the pressing plate will be pressed into indentations and should be adjusted.


10. What is the reason for the change in the position of the blank hole during bending? How to exclude

A. The position and size of the hole are incorrect, resulting in thinning due to bending and stretching

Measures: Strictly control the bending radius, bending angle, and material thickness; Trim the neutral layer of the material so that the depth of the convex mold entering the concave mold and the depth of the convex and concave molds are appropriately consistent.

B. Reasons for non concentric holes

1) Insufficient bending height. 2) The blank slides. 3) Rebound. 4) The curved plane exhibits undulations.

measures:

1) Ensure the correct left and right bending height.

2) Correct the worn positioning pins and plates.

3) Reduce rebound and ensure the parallelism and flatness of the two curved surfaces.

4) Change the process route, first bend and correct before punching.

C. The bending curve is not parallel to the centerline of the two holes, and the part with a bending height less than the minimum bending height shows an outward opening shape after bending.

measures:

1) When bending, the minimum bending height H (H ≥ R 2t t material thickness R bending radius) should be ensured.

2) Change the shape of the processed parts and remove parts with a bending height less than the minimum without affecting their use.

D. Holes near curved lines are prone to deformation.

measures:

1) When designing bent parts, ensure that the edge distance X from the bent part to the hole is greater than a certain value X ≥ (1.5-2.0) t t t of the bent sheet thickness.

2) Designing auxiliary holes in the bending area to absorb bending deformation stress can prevent hole deformation near the bending curve. Generally, the scheme of bending first and punching later is adopted.


11. After bending, the bent parts show significant thinning

A. The bending radius is too small relative to the plate thickness value (r/t>3 right angle bending). Generally, increasing the bending radius is used.

B. Multi angle bending makes the bent part thinner and larger. In order to reduce thinning, the single angle multi process bending method should be used as much as possible.

C. When using a pointed convex mold, the convex mold enters the concave mold too deeply, significantly reducing the thickness of the bent part.


12. Reasons and prevention of flange wrinkling during deep drawing process of deep drawn parts

reason:The edge pressure on the flange is too small to resist excessive tangential compressive stress; And it causes tangential deformation, resulting in the formation of folds after losing stability. Thinner materials are also prone to wrinkle formation.

measures:Increase the edge pressure of the edging ring and appropriately increase the thickness of the material.


13. Reasons and prevention of wall cracking in deep drawn parts

reason:

A. Excessive radial tensile stress of the material during stretching;

B. The radius of the concave mold fillet is too small,

C. Poor lubrication during deep drawing;

D. The plasticity of raw materials is poor.

measures:

1) Reduce the edge pressure.

2) Increase the fillet radius of the concave mold.

3) Proper use of lubricants.

4) Choose materials with better performance or add annealing processes in the workshop.


14. The bottom of the deep drawn part is cracked by pulling

The reason is that the fillet radius of the concave mold is too small, which causes the material to be cut. (Usually occurring in the early stage of deep drawing) Increasing the fillet radius of the concave die reduces the surface roughness of its smooth transition, usually Ra<0.2 μ m.


15. The edges of the deep drawn parts are uneven and wrinkled.

reason:The blank and the center of the convex concave die are not in a straight line or the material thickness is uneven. The radius of the concave die corner is uneven with the gap between the convex concave die (if the radius of the concave die corner is too large, the edge pressing ring and the edge pressing ring will separate in the final stage of deep drawing, and the material that does not cross the corner cannot be pressed into the edge pressing ring and wrinkled before being pulled into the concave die to form mouth edge wrinkles).

measures:Repositioning the die, before putting it into production, adjust the fillet radius of the concave die and the clearance between the convex and concave dies to make them uniform in size (reducing the fillet radius of the concave die or using an arc-shaped edge pressing ring device can remove wrinkles)


16. Reasons and preventive measures for wrinkling at the waist during deep drawing of conical or hemispherical parts:

reason:At the beginning of deep drawing, most of the material is in a suspended state, with too little edge pressure, too large fillet radius of the die, or excessive use of lubricant. The radial tensile stress decreases, and the material loses stability under tangential compressive stress, resulting in wrinkles.

measures:Increase the edge pressure or adopt a rolled rib structure, reduce the fillet radius of the concave die or slightly increase the material thickness.


17. Reasons and preventive measures for drawing marks on the surface of deep drawn parts

reason:

A. If there are sharp scratches on the surface of the convex or concave mold, resulting in corresponding tensile marks on the surface of the workpiece, the surface should be polished or buffed.

B. The gap between the convex and concave molds is too small or uneven, causing scratches on the surface of the workpiece during deep drawing. At this time, the gap between the convex and concave molds should be adjusted until it is suitable.

C. The concave die has a rough rounded surface, and the workpiece surface is scratched during stretching. At this point, the radius of the rounded corners of the concave mold should be polished and smoothed.

D. During stamping, impurities are mixed into the working surface or material surface of the die due to uncleanliness, which damages the surface of the workpiece. Therefore, the surface of the convex and concave molds must always be kept clean during material pulling, and the blank must be wiped before pulling;

E. When the hardness of the convex and concave molds is low, metal shavings will adhere to their surfaces, and there will also be stretch marks on the surface of the deep drawn workpiece. Therefore, in addition to increasing the hardness of the convex concave die surface, even if the remaining metal waste is removed, the surface of the convex concave die should always be inspected.

F. Poor quality lubricants can also increase the surface roughness of deep drawn workpieces. In this case, lubricants suitable for deep drawing processes should be used, and if necessary, the lubricant should be filtered before use. Thus preventing impurities from entering and damaging the surface of the workpiece.


18. What is the reason for the unevenness of the straight wall of the deep drawn part?

reason:

A. There are no ventilation holes designed and manufactured on the convex mold, so the surface of the convex mold will deform due to compressed air, resulting in unevenness. In this case, ventilation holes must be added.

B. The rebound of the material can also cause unevenness on the surface of the deep drawn workpiece, and finally, a shaping process needs to be added.

C. The gap between the convex and concave molds is too large, making it difficult to flatten during deep drawing. At this time, the gap must be uniformly adjusted.

News Related news
中文字幕一区二区视频 | 在线免费观看黄 | 久久久视屏 | 日韩视频区| 黄色精品免费 | 国产精品极品白嫩在线 | 亚洲国产在 | 亚洲色图 校园春色 | 国产精品激情偷乱一区二区∴ | 亚洲网色 | www.中文字幕在线观看 | 欧美成人精品激情在线视频 | 少妇免费毛片久久久久久久久 | 99久久久无码国产精品性黑人 | 一级免费看 | 欧美三级午夜理伦三级 | 色呦呦视频 | 午夜色av | 久草久 | 精品国产制服丝袜高跟 | 8x8x国产精品一区二区 | 激情五月俺也去 | 少妇 av| 久热中文字幕 | 亚洲天堂一区在线观看 | 日韩视频中文 | 精品国产乱码久久久久久预案 | 日本中文字幕在线播放 | 91麻豆免费看 | 4438全国最大成人网 | 名校风暴在线观看免费高清完整 | 欧美色涩在线第一页 | 日本十八禁视频无遮挡 | 中文在线播放 | 免费国产一区 | 国产精品久久久久久久久夜色 | 成人免费短视频 | 天天做天天爱天天爽 | 内射国产内射夫妻免费频道 | 中文字幕精品久久久久人妻红杏1 | 日韩污视频 | 国产麻豆免费视频 | 能看的毛片 | 图片区 小说区 区 亚洲五月 | 国产激情在线播放 | 激情综合丁香五月 | 白嫩初高中害羞小美女 | 欧美色图亚洲激情 | 中文字幕在线永久 | 国产一区999 | 日韩在线观看第一页 | 国产极品美女在线 | 5a毛片| 性色在线 | 狠狠a | 美妇湿透娇羞紧窄迎合 | 九月丁香婷婷 | 亚洲精品传媒 | av有码在线观看 | 国产在线视频导航 | 日韩精品一区二区av | 美女aaa| 欧美成人午夜免费视在线看片 | 午夜视频在线观看免费视频 | 伊人一道本| 最近中文字幕在线中文高清版 | 日韩porn| 在线观看免费视频国产 | 日剧网 | 免费黄色av网站 | 孕妇爱爱视频 | 久久精品欧美一区二区三区麻豆 | 欧美日韩三区 | 黄色在线播放网站 | 人妻精品无码一区二区三区 | 国产在线观看一区二区三区 | 又欲又污又肉又黄短文 | 青草视频免费在线观看 | 欧美四虎| 午夜精品久久久久久久第一页按摩 | www视频在线免费观看 | 激情偷乱人成视频在线观看 | 亚洲一区二区三区黄色 | 国产精品一卡 | 亚洲国产精品久久久 | 日韩av在线网 | 黄色片hd | 欧美一级片观看 | 欧美日韩一级二级 | 国产99在线播放 | 人与拘一级a毛片 | 日韩高清中文字幕 | 日本高清xxx | 一级片免费在线播放 | 日韩黄色大全 | 另类第一页 | 国产我不卡 | 成人在线免费网站 | 日本爽妇网 | 日本在线视频一区二区三区 | 91视频首页 | 在线观看国产三级 | 九九热精品在线观看 | www.亚洲色图| 色呦呦呦呦 | 91吃瓜在线 | 日本美女性爱视频 | 少妇一晚三次一区二区三区 | 精品国产av 无码一区二区三区 | 男女插鸡视频 | 人成午夜 | 国产精品美女久久久久av超清 | 久久精品h | 成人动漫视频在线观看 | 日本在线观看中文字幕 | 夜夜躁日日躁狠狠久久av | 天天撸天天射 | 欧美一级在线观看 | 综合视频| 黄瓜视频在线免费看 | 国产乱国产乱 | 日韩在线二区 | 精品少妇爆乳无码av无码专区 | 97视频免费在线 | 日本免费一二区 | 国产精品亚洲AV色欲三区不卡 | 久草免费福利 | 中文亚洲av片在线观看 | 国产91精品一区 | 国产每日更新 | 深夜福利一区二区 | 国产精品黄色网 | 黄色理伦片 | 97超碰人人 | 日韩在线不卡 | 人人97 | 91操操| 国产片天天弄 | 中文字幕永久免费 | 国产精品.xx视频.xxtv | 视频一区在线播放 | 麻豆视频在线免费观看 | 久操网站 | a在线播放| 国产经典一区二区三区 | 久久r精品| 亚洲精品中文字幕乱码三区91 | 99午夜| 亚洲香蕉在线视频 | 亚洲综合免费观看高清完整版 | 丰满人妻一区二区三区性色 | 四虎免费影视 | 国产成人aaaa | 中文字幕人妻精品一区 | 麻豆网站免费看 | 国产精品夜夜夜爽阿娇 | 少妇高潮网站 | 精品盗摄一区二区三区 | 麻豆视 | 男男做爰猛烈啪啪高 | 久操视频在线观看 | a级国产毛片 | 在线观看av大片 | 波多野结衣免费观看视频 | 福利小视频在线播放 | 欧美成人精品一区二区三区 | 小情侣高清国产在线播放 | 国产va| 亚洲 精品 综合 精品 自拍 | 在线观看免费高清在线观看 | 国产日韩精品一区二区三区在线 | 国产大片黄 | 欧美九九九 | 国产精品日韩欧美一区二区三区 | 亚洲精品久久久久久久久久久 | 亚洲乱码一区二区三区在线观看 | 国产福利三区 | 顶级黑人搡bbw搡bbbb搡 | 亚洲av无码片一区二区三区 | 自拍偷拍视频在线 | 亚洲精品色午夜无码专区日韩 | 91国在线观看 | 日韩成人精品在线观看 | china国产乱xxxxx绿帽 | 肉色丝袜脚交一区二区 | 亚洲人成电影一区二区在线 | 翔田千里x88aⅴ | 亚洲精品一线 | 国产成人精品一区二区三区四区 | 夜色一区二区 | 国产人与禽zoz0性伦 | 国产传媒视频 | 风间由美一二三区av片 | 国产精品66 | 日本三级韩国三级三级a级中文 | 亚洲激情视频在线观看 | 成人精品在线视频 | 四虎网站最新网址 | 久久免费av | 久久久久久久久国产精品 | 狠狠噜噜 | 国产吞精囗交免费视频网站 | 免费www xxx| 欧美一级在线视频 | 亚洲另类天堂 | www.xxx.日本 | 国产精品亚洲色图 | 岛国av不卡 | 精品人妻一区二区三区含羞草 | 精品无码成人久久久久久免费 | 成人小视频免费 | 欧美黑人巨大xxx极品 | 日韩欧美在线观看一区二区三区 | 精品91久久久久久 | 日韩一级不卡 | 97超碰中文| 亚洲精品播放 | 色播视频在线播放 | 激情四射综合网 | 国产又粗又长又黄视频 | 欧美91视频| 天天久 | 东北女人av| 国产主播一区 | 免费毛片网站在线观看 | 婷婷射图 | 国产精品99精品无码视 | 操女人免费视频 | 免费成人美女女 | 天堂网免费视频 | 爱插美女网| 精品人妻无码一区二区性色 | 超碰免费在线 | 国产精品视频一二三 | 性生活视频软件 | 欧美第一页浮力影院 | 久热在线视频 | 潘金莲三级野外 | 国产噜噜噜噜噜久久久久久久久 | 免费看国产黄色 | 日本老太婆做爰视频 | 午夜精品久久久久久久 | 精品人妻无码一区二区三区蜜桃一 | 一区二区三区久久久 | www中文字幕 | 极品在线观看 | 亚洲成人三区 | 色屁屁在线 | 国产精品四虎 | 久热热 | 色偷偷资源网 | 老司机午夜免费精品视频 | 日本东京热一区二区三区 | 激情久 | 视频在线看 | 色爽影院| 天天想你在线观看完整版电影高清 | 波多野结衣一区二区三区高清av | 国产伦精品一区三区精东 | 国产熟女一区二区丰满 | 天天草比 | 狼人伊人干| 亚洲色图偷拍 | 亚洲欧洲成人精品久久一码二码 | 欧美性生活| 少妇又色又爽又黄的视频 | 欧美大片视频在线观看 | 狠狠爱av | 国产精品欧美综合亚洲 | 日韩一区二区视频 | 俄罗斯色片 | 国产88av| 日韩av一二区 | 免费一级黄色 | 男人天堂新地址 | 麻豆av免费在线 | 五月婷婷在线观看 | 亚洲一二三四视频 | 成人免费无遮挡无码黄漫视频 | 国产精品久久久久一区二区 | 波多野结衣一区二区 | 久久精品亚洲一区 | 狠狠v欧美v日韩v亚洲ⅴ | 久久国产色av免费观看 | 网站免费黄色 | 亚洲91网| 黄瓜视频在线观看污 | caopor超碰 | 伊人久久爱 | 77久久| 国产69页 | 久久精品美女 | 99re国产精品 | 日韩精品福利视频 | 日本啪啪网 | 激情综 | 亚洲人人夜夜澡人人爽 | 成人精品福利视频 | 免费看黄20分钟 | 天堂在线中文字幕 | 日韩a级黄色片 | av图区| 岳乳丰满一区二区三区 | 中国浓毛少妇毛茸茸 | 精品少妇v888av | 性一交一乱一透一a级 | 精品人妻伦九区久久aaa片 | 日韩欧美成人精品 | 九九热视频在线观看 | 国产一级高清视频 | 全部孕妇毛片 | 欧美亚洲免费 | 欧美日韩国产综合网 | 欧美毛茸茸 | 好男人www日本 | 日韩亚洲精品视频 | 日韩精品视频在线 | 久久久久久久久久一区二区三区 | 男女性生活视频网站 | 天天爽夜夜爽夜夜爽精品视频 | 美女福利影院 | 长篇高h肉爽文丝袜 | 成人欧美一区二区三区在线观看 | 一区二区手机在线 | 成年在线观看 | 午夜精品久久久久久久96蜜桃 | 超碰97成人| 欧洲一区在线观看 | 国产成人av免费 | 国产中文字幕一区二区 | 亚洲国产精品午夜久久久 | 欧美激情国产在线 | 先锋影音av中文字幕 | 爱爱网视频 | 一区二区视频国产 | 91国产丝袜播放在线 | 一区二区日韩电影 | 97免费人妻无码视频 | 欧美精品欧美极品欧美激情 | 青青免费视频 | 日韩3区| 91久久国语露脸精品国产高跟 | 欧美日韩一区二区三区四区五区 | 91五月天 |